EVA extrusion melt fracture

Sorun Belirtisi
Severe melt fracture occurs when EVA extrusion rate is too high, with extrudate twisted in spiral shape
Neden Analizi
EVA melt elasticity too high with elastic recovery at die exit exceeding critical value; die L/D ratio too short <10 with melt not fully relaxed; extrusion temperature too low
Çözüm
1) Reduce extrusion rate to 2-3m/min; 2) Increase die L/D ratio to 15-20; 3) Increase extrusion temperature to 140-200°C; 4) Add small amount of low-elasticity resin to reduce system elasticity; 5) Progressive converging die entrance design
Temel Çıkarım
Melt fracture is caused by elastic recovery exceeding critical value; reducing speed and lengthening die are the core countermeasures