Material Drying
5 görüntüleme
CEF '2079851475616104452 thick-wall bubbles
Sorun Belirtisi
CEF injection molded thick-wall products have dense bubbles 0.1-0.5mm inside, concentrated in the wall thickness center
Neden Analizi
Insufficient holding pressure <40MPa or short holding pressure time, thick wall center not compacted; raw material contains moisture; injection speed too fast, air entrained; poor mold venting
Çözüm
1) Increase holding pressure to 60-80MPa; 2) Extend holding pressure time so the thick wall is fully compacted; 3) Fully dry the raw material, moisture <0.02%; 4) Add vent grooves or vent pins to the mold; 5) Progressive deceleration injection to avoid air entrainment
Temel Çıkarım
Thick-wall bubbles are caused by a combination of insufficient holding pressure, moisture, and poor venting
Bu faydalı oldu mu?
0 kişi bunu faydalı buldu
Geri bildiriminiz için teşekkürler!