Production & Quality
12 görüntüleme
CEF repeated processing performance decay
Sorun Belirtisi
After CEF is recycled and reprocessed 3-4 times, the tensile strength decreases by 25-30%
Neden Analizi
Molecular chains break and degrade under repeated high-temperature shearing; the antioxidant is exhausted in multiple processing; cumulative effect of thermo-mechanical degradation
Çözüm
1) The proportion of recycled material does not exceed 20-30%; 2) Supplement 0.1-0.2wt% antioxidant for each re-extrusion; 3) Reduce the processing temperature by 5-10°C; 4) Reduce the screw speed to reduce shearing
Temel Çıkarım
The performance decay of multiple processing is caused by thermo-mechanical degradation; limiting recycled material and supplementing antioxidants are the key
Bu faydalı oldu mu?
0 kişi bunu faydalı buldu