Production & Quality 14 visualizações

CEF repeated processing performance decay

Fenómeno do problema
After CEF is recycled and reprocessed 3-4 times, the tensile strength decreases by 25-30%
Análise das causas
Molecular chains break and degrade under repeated high-temperature shearing; the antioxidant is exhausted in multiple processing; cumulative effect of thermo-mechanical degradation
Solução
1) The proportion of recycled material does not exceed 20-30%; 2) Supplement 0.1-0.2wt% antioxidant for each re-extrusion; 3) Reduce the processing temperature by 5-10°C; 4) Reduce the screw speed to reduce shearing
Conclusão principal
The performance decay of multiple processing is caused by thermo-mechanical degradation; limiting recycled material and supplementing antioxidants are the key
CEF recyclingperformance decayantioxidant supplementationthermal degradationshear degradation

Isto foi útil?

0 pessoas acharam isto útil

ChemAI