Sorun Belirtisi
MP extruded product surface roughness Ra>5μm, exceeding the requirement
Neden Analizi
extrusion temperature low <150°C, melt flow unstable; die inner wall rough or damaged; MP melt elasticity, extrusion swell uneven
Çözüm
1) raise extrusion temperature to 150-170°C; 2) polish die inner wall Ra<0.4μm; 3) reduce extrusion rate 10-15%; 4) add 0.3-0.5wt% external lubricant
Temel Çıkarım
rough surface is caused by low-temperature extrusion and die defects; raising temperature and polishing the die are the core countermeasures
MP extrusion rough surface die polishing extrusion temperature melt elasticity