Extrusion & Post 5 görüntüleme

Unstable frost line height of low density polyethylene film

Sorun Belirtisi
The frost line height of blown film fluctuates greatly, film thickness and quality unstable. Frost line height reflects cooling condition stability, directly affecting film performance.
Neden Analizi
(1) Unstable air ring air volume or air speed (2) Extrusion temperature fluctuation (3) Ambient airflow interference (4) Screw rotation speed fluctuation (5) Cooling air temperature fluctuation
Çözüm
(1) Check air ring blower and valves, ensure stable air volume (2) Stabilize extrusion temperature, control fluctuation within ±3°C (160-220°C range) (3) Install wind shields or isolation curtains, reduce ambient airflow interference (4) Stabilize screw rotation speed (5) Use constant temperature cooling air, reduce temperature fluctuation
Temel Çıkarım
Unstable frost line is caused by fluctuating cooling or extrusion conditions; air ring parameters and environmental conditions need to be stabilized.
cooling linefrost lineair ring stabilityextrusion temperatureambient airflow