Extrusion & Post
6 مشاهدة
LLDPE Blown Film Poor Plasticization (Unmelted Particles)
ظاهرة المشكلة
White unplasticized particle points appear on the film surface, especially obvious on stretch film.
تحليل الأسباب
LLDPE has high viscosity and is difficult to plasticize, and ordinary screws with insufficient mixing produce unmelted particles; they appear in batches when output is too high beyond the plasticization capacity.
الحل
① Use a special screw with barrier section + mixing section; ② reduce output or raise barrel temperature; ③ use finer filter screens to intercept; ④ check screw wear.
الخلاصة الأساسية
LLDPE has the highest requirements for screw mixing, and ordinary screws are not enough.
هل كان هذا مفيدًا؟
0 شخص وجدوا هذا مفيدًا