Molds & Tooling 9 مشاهدة

POM dimensions continue to shrink after demolding

ظاهرة المشكلة
Products measure acceptable at demolding, but re-measurement after 24 hours shows dimensions are significantly smaller, and assembly reveals fits that are too tight or loose.
تحليل الأسباب
POM has high crystallinity, and crystallization continues after demolding, producing post-shrinkage that can last more than 24 hours; high demolding temperature and uneven mold temperature increase the post-shrinkage amount.
الحل
①Let products stabilize for 24 hours before measuring for inspection; ②design the mold with about 2.8% shrinkage compensation; ③extend in-mold cooling for shaping; ④stabilize mold temperature to reduce fluctuation.
الخلاصة الأساسية
POM post-shrinkage is an inherent material characteristic; dimensional judgment must be made after sufficient aging, and mold compensation and cooling shaping must reserve shrinkage allowance.; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
POM;post-shrinkage;dimension;crystallization;aging;shrinkage