Extrusion & Post 12 مشاهدة

MP extruded profile bending deformation

ظاهرة المشكلة
MP extruded profiles continuously bend after cooling, bending deviation >5mm/m
تحليل الأسباب
uneven cooling on each surface of the profile causes shrinkage difference; uneven die exit flow velocity makes profile wall thicknesses different; haul-off and extrusion centerlines misaligned producing lateral force
الحل
1) optimize the cooling system to ensure uniform cooling on all surfaces; 2) adjust the die so each wall has uniform flow velocity and consistent wall thickness; 3) align haul-off and extrusion centerlines; 4) increase calibrating sleeve length, cool after full calibration
الخلاصة الأساسية
profile bending is caused by uneven cooling and uneven flow velocity; homogenization and alignment are the keys to solving