Extrusion & Post
12 مشاهدة
MP extruded film gel particles
ظاهرة المشكلة
MP extruded film surface shows 0.1-0.5mm transparent gel particles
تحليل الأسباب
high molecular weight components in MP not fully melted during extrusion, forming local high-crystallinity zones; extrusion temperature low or mixing insufficient
الحل
1) raise extrusion temperature 5-10°C to ensure full melting; 2) increase screw mixing section length; 3) inspect raw material to ensure consistent grade; 4) replace with a finer screen 120 mesh to intercept unmelted particles
الخلاصة الأساسية
gel particles are caused by incomplete melting; raising temperature and mixing are key