Extrusion & Post
14 visualizaciones
MP extruded film gel particles
Fenómeno del problema
MP extruded film surface shows 0.1-0.5mm transparent gel particles
Análisis de la causa
high molecular weight components in MP not fully melted during extrusion, forming local high-crystallinity zones; extrusion temperature low or mixing insufficient
Solución
1) raise extrusion temperature 5-10°C to ensure full melting; 2) increase screw mixing section length; 3) inspect raw material to ensure consistent grade; 4) replace with a finer screen 120 mesh to intercept unmelted particles
Conclusión clave
gel particles are caused by incomplete melting; raising temperature and mixing are key
¿Le ha resultado útil?
0 personas encontraron esto útil
¡Gracias por sus comentarios!