Material Drying
6 مشاهدة
Bubbles in PLA '2079851475616104452 after moisture absorption
ظاهرة المشكلة
Bubbles appear on the surface and inside of PLA products.
تحليل الأسباب
PLA has strong hygroscopicity; when drying is insufficient, the moisture content is high (>500ppm), and water vapor produces bubbles during processing.
الحل
Drying conditions: 60-80°C/4-6h (amorphous grade) or 80-100°C/2-3h (crystalline grade) to moisture <250ppm.
الخلاصة الأساسية
The hygroscopicity of PLA is the first obstacle to processing quality.