Extrusion & Post
10 Aufrufe
PVC Extrusion Pipe Temperature
Problembeschreibung
Extruded PVC pipe inner wall rough, surface sharkskin, or degraded yellow lines
Ursachenanalyse
Improper extrusion temperature zoning: feed zone 60-80℃ preheating, compression zone 140-150℃ plasticizing, metering zone 160-170℃ homogenizing, die head 170-180℃ shaping; local overheating immediately gives yellow lines
Lösung
①Set and stabilize according to zoned temperature curve; ②Uniform die head temperature to prevent yellow lines; ③Screw speed matched with haul-off; after adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability
Wichtigste Erkenntnis
PVC pipe extrusion is the art of zoned temperature control; each zone has its duty, local overheating immediately shows; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
War das hilfreich?
0 Personen fanden dies hilfreich
Vielen Dank für Ihr Feedback!