MP compression molded product bubbles

Problembeschreibung
MP melamine tableware compression molded products have surface bubbles 0.5-2mm
Ursachenanalyse
preform powder contains moisture >0.5%; insufficient venting, air and volatiles in the mold cavity cannot escape
Lösung
1) dry preform powder at 80°C for 2h to moisture <0.1%; 2) add vent grooves to the mold; 3) pre-press degassing 1-2 times to release volatiles
Wichtigste Erkenntnis
MP compression molding bubbles are caused by moisture and poor venting; drying and venting are key