Material Drying 2 views

MP compression molded product bubbles

Problem Phenomenon
MP melamine tableware compression molded products have surface bubbles 0.5-2mm
Cause Analysis
preform powder contains moisture >0.5%; insufficient venting, air and volatiles in the mold cavity cannot escape
Solution
1) dry preform powder at 80°C for 2h to moisture <0.1%; 2) add vent grooves to the mold; 3) pre-press degassing 1-2 times to release volatiles
Key Takeaway
MP compression molding bubbles are caused by moisture and poor venting; drying and venting are key
MP compression molding bubble preform powder drying vent groove pre-press degassing