Molds & Tooling 4 visualizaciones

ASA thick wall sink mark

Fenómeno del problema
ASA product thick-wall areas and rib backs show depressed sink marks, surface defects unacceptable for automotive exterior parts, flash appears at edges after increasing holding pressure.
Análisis de la causa
Thick-wall area cools unevenly and outer layer solidifies first, internal shrinkage with insufficient feeding forms depression; ASA shrinkage rate 0.4~0.7% is low, but local thick-wall shrinkage concentration still exceeds appearance tolerance; holding pressure transmission is limited by gate freezing.
Solución
①Increase holding pressure and time to compensate thick-wall shrinkage; ②design rib wall thickness at 50~60% of main wall; ③move gate near thick-wall area; ④solve the balance between holding pressure and flash with multi-stage holding pressure.
Conclusión clave
ASA sink mark governance emphasizes both holding pressure and structural design; rib thickness ratio is a design red line; multi-stage holding pressure resolves the contradiction between sink mark and flash.; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
ASA; sink mark; thick wall; holding pressure; rib; flash