Molds & Tooling 7 visualizaciones

PC/ABS Sink Marks

Fenómeno del problema
PC/ABS products have depressions on the back of ribs, obvious on the appearance surface.
Análisis de la causa
Insufficient holding pressure or the gate freezing too early means thick-section shrinkage is not compensated; an excessive rib thickness ratio aggravates it; although PC/ABS shrinks less than crystalline materials, thick-wall areas still have sink marks.
Solución
①Gradually increase holding pressure and time; ②Confirm the gate open time is sufficient; ③Control rib thickness to within about 50% of wall thickness; ④Core out and reduce material at thick-wall areas to reduce shrinkage from the source; ⑤Strengthen local cooling.
Conclusión clave
PC/ABS sink marks 'first add holding pressure, then check rib thickness': as a low-shrinkage material, sink marks mostly stem from structural wall thickness and holding pressure management; only by emphasizing both process and structure can it be radically cured.
PC/ABS; sink mark; holding pressure; rib thickness; freeze