Material Drying 7 visualizaciones

PLA High-Temperature Processing 50ppm

Fenómeno del problema
PLA products processed at high temperature or with long residence become more severely brittle; the same drying conditions fail
Análisis de la causa
When the processing temperature is higher than 240℃ or the residence time is long, the hydrolysis degradation window is wider, and the moisture requirement tightens from 100ppm to below 50ppm to avoid a decrease in number-average molecular weight
Solución
①For high-temperature processes, tighten the drying standard to 50ppm; ②Shorten the melt residence time; ③Re-evaluate the drying capacity for processes exceeding 240℃; after adjustment, take continuous samples to verify the effect, and resume mass production only after confirming stability
Conclusión clave
PLA's moisture red line tightens with temperature; processes above 240℃ must implement 50ppm-level ultra-strict drying; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
PLA; 50ppm; 240℃; residence; high temperature