Molds & Tooling
7 visualizaciones
PMMA Vent Groove Depth Improper
Fenómeno del problema
After adding vent grooves, flash appears at product edges, or vent grooves are too shallow and trapped-air burning remains unsolved.
Análisis de la causa
When vent groove depth exceeds 0.04mm, PMMA melt penetrates to form flash; if depth is less than 0.02mm, venting is poor and the trapped-air problem remains.
Solución
①Control vent groove depth at 0.02~0.04mm; ②densify venting points according to defect locations; ③regularly clean accumulated material in vent grooves; ④verify venting effectiveness.
Conclusión clave
Vent groove depth is a fine parameter of PMMA molds; take the specification range between preventing flash and ensuring venting, and arrange with emphasis at filling ends.; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence.