Extrusion & Post 9 visualizaciones

PP Sheet Die Lip Buildup

Fenómeno del problema
After a period of PP sheet extrusion, material hangs on the die lip, and periodic longitudinal streaks or lines appear on the sheet surface.
Análisis de la causa
Melt stagnates and degrades at the die lip exit edge, gradually building up into deposit that periodically sheds and is pressed into the sheet surface; high raw material volatiles and mismatched exit temperature and line speed accelerate buildup.
Solución
①Regularly clean die lips with tools such as copper brushes; ②optimize exit zone temperature to avoid local overheating degradation; ③appropriately reduce line speed; ④check raw '2079851475616104451 and regrind ratio; ⑤evaluate adding processing aids to reduce stagnation.
Conclusión clave
PP die lip buildup is an accumulation process of 'stagnation degradation': cleaning treats the symptom, while temperature-speed matching treats the root; the interval pattern of periodic streaks from buildup can back-calculate the buildup shedding cycle.
PP;extrusion;die lip buildup;mold deposit;stagnation;streak