Extrusion & Post 10 visualizaciones

PSU Annealing Process for Stress Relief

Fenómeno del problema
[Problem Phenomenon] PSU precision parts show dimensional drift and crazing in solvent environments; no annealing treatment was performed
Análisis de la causa
Annealing can improve PSU physical aging and solvent crazing and reduce molding internal stress; a 150°C×2-4h annealing procedure is recommended; hot mold molding can also reduce internal stress
Solución
Anneal products at 150°C×2-4h after demolding and cool slowly; use hot molds during molding to reduce stress generation; annealing is mandatory before plating and bonding; after adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability
Conclusión clave
150°C×2-4h annealing is a standard action for PSU stress management and cannot be omitted; After confirming effectiveness, solidify the parameters and practices into the work instructions to prevent recurrence
annealing 150°C solvent crazing dimensional stability