Extrusion & Post
14 visualizaciones
Unstable dimensions in EAA extrusion
Fenómeno del problema
The cross-sectional dimensions of EAA extruded products fluctuate ±10%, and there are also periodic changes in the length direction
Análisis de la causa
Unstable feeding amount, fluctuation of feeding screw speed; periodic fluctuation of extrusion temperature ±5°C; haul-off speed does not match the extrusion speed
Solución
1) Use a loss-in-weight feeder to ensure stable feeding; 2) PID control of each extruder zone temperature with accuracy ±1°C; 3) Closed-loop control of haul-off speed linked with extrusion speed; 4) Control the processing temperature at 180-240±5°C
Conclusión clave
Extrusion dimensional stability depends on feeding accuracy, temperature control and haul-off synchronization