Extrusion & Post 14 visualizaciones

DSTDP blended with incompatible resins delamination

Fenómeno del problema
DSTDP blended with polar resins such as PA/ABS, extrudate completely delaminates, mechanical properties extremely poor
Análisis de la causa
DSTDP and polar resins have large polarity difference, compatibility is zero, interfacial adhesion extremely low, no compatibilizer used
Solución
1) Use DSTDP graft compatibilizer DSTDP-g-MAH 2-5wt%; 2) add epoxy-type compatibilizer 1-2wt%; 3) keep DSTDP addition <10wt% to keep the other resin as the continuous phase; 4) twin-screw high-shear compounding to disperse DSTDP <0.3μm
Conclusión clave
Blends with large polarity differences require reactive compatibilizers that form chemical bonding at the interface to solve