Extrusion & Post 14 visualizaciones

DSTDP extruded film poor thickness uniformity

Fenómeno del problema
DSTDP extruded film transverse thickness deviation ±15%, exceeding the ±5% industry standard
Análisis de la causa
Unreasonable die flow channel design causes uneven melt flow in the wide die; DSTDP melt elasticity large, extrusion swell uneven; air ring cooling uneven
Solución
1) Adopt coat-hanger die design to ensure uniform transverse flow; 2) fine-adjust die gap ±0.02mm; 3) optimize air ring air volume and angle for uniform cooling; 4) add a small amount of low-elasticity resin to reduce swell difference
Conclusión clave
Film thickness uniformity needs coordinated optimization from the three aspects of die design, gap adjustment and cooling
DSTDP filmthickness uniformitydie designextrusion swellair ring cooling