Extrusion & Post 14 visualizaciones

DSTDP film poor print adhesion

Fenómeno del problema
DSTDP film ink adhesion after printing <2 grade, cross-cut test large-area peeling off
Análisis de la causa
DSTDP surface polarity has poor affinity with ink; corona treatment effect decays fast; ink system not matched with DSTDP
Solución
1) Print immediately after corona treatment within 24h; 2) use DSTDP-specific ink; 3) increase corona power to 15-20kW/m² to ensure surface tension >42mN/m; 4) flame treatment to assist surface polarization
Conclusión clave
Poor print adhesion is caused by insufficient surface polarity; corona treatment and special ink are key
DSTDP filmprint adhesioncorona treatmentspecial inksurface tension

¿Le ha resultado útil?

0 personas encontraron esto útil

ChemAI