Extrusion & Post 12 visualizaciones

Uneven thickness of polyolefin plastomer cast films

Fenómeno del problema
The transverse thickness deviation of the cast film is large, exceeding the tolerance range. Uneven thickness affects the winding quality of the film and subsequent processing, and affects service performance in precision films.
Análisis de la causa
(1)The lip gap of the T-die is uneven (2)The die temperature distribution is uneven (3)The air knife airflow is uneven (4)The cooling roller temperature is uneven (5)The extrusion output fluctuates
Solución
(1)Adjust the lip gap of the T-die, using a feeler gauge to check uniformity (2)Check the die heater distribution to ensure the transverse temperature difference does not exceed ±3°C (180-230°C range) (3)Check the air knife to ensure uniform air output, and clean the air knife opening (4)Check the temperature uniformity of the cooling roller, with the temperature difference not exceeding ±2°C (5)Stabilize the extruder screw speed and temperature
Conclusión clave
Uneven cast film thickness is caused by uneven die gap or temperature, and needs to be solved from mold precision and temperature uniformity.
cast filmuneven thicknessT-dielip gapair knife