Molding Process
5 조회수
PMMA Sink Marks
문제 현상
Depressions on the back of thick walls and ribs, appearing as optical distortion in transparent parts.
원인 분석
Uneven wall thickness + insufficient feeding; hard pressure feeding in turn increases internal stress and induces delayed cracking.
해결 방법
①Uniform wall thickness (0.635~3.81mm); ②Rib thickness ≤50%~60%; ③Moderate holding pressure; ④Reduce material in thick walls.
핵심 요약
PMMA sink marks rely on structure, hard pressure trades for delayed cracking.