Molding Process
7 조회수
EVA foam open cell content is high
문제 현상
EVA foam open cells >30%, exceeding 10%
원인 분석
Foaming temperature too high with thin cell walls rupturing into open cells; insufficient crosslinking with low wall strength
해결 방법
1) Reduce temperature by 5-10°C to reduce wall rupture; 2) DCP 0.5-0.8wt% to increase wall strength; 3) Appropriately reduce AC to reduce gas pressure impact
핵심 요약
High open cell content is caused by cell wall rupture; temperature control and moderate crosslinking are key