EAA surface orange peel texture

Problem Phenomenon
Orange-peel-like uneven texture on the EAA product surface with rough hand feel
Cause Analysis
Mold temperature too low <30°C, product surface cools and solidifies rapidly while the interior continues to shrink, causing surface unevenness; injection speed too low
Solution
1) Increase mold temperature to 40-50°C to delay surface solidification; 2) Appropriately increase injection speed; 3) Increase holding pressure to reduce internal shrinkage
Key Takeaway
Orange peel texture is caused by rapid cooling and solidification; increasing mold temperature and holding pressure is key