MP '2079851475616104452 mold venting burning

Problem Phenomenon
MP injection mold venting insufficient, air in the cavity compressed and heated causing local burning
Cause Analysis
mold vent groove area insufficient or position improper; injection speed too fast, air has no time to escape; air compressed to high temperature >200°C causing oxidative burning
Solution
1) increase vent groove area, depth 0.02-0.03mm, width 5-10mm; 2) locate vent grooves at the last-filled region of the melt; 3) reduce injection speed to reduce air compression; 4) multi-stage injection with slow advance for venting
Key Takeaway
burning is caused by insufficient venting and high-speed injection compressing air; increasing venting and reducing speed are key