PET Preform Neck White Spot Crystallization

Fenómeno do problema
White crystallization spots appear on the threaded neck of the preform, affecting the neck appearance and sealing fit; after blowing, the white spot area is still white.
Análise das causas
Too slow injection speed causes the melt front to cool and crystallize at the neck; sudden injection speed changes, melt viscosity too high or low mold temperature at the neck area all make the melt unable to fill quickly.
Solução
①Increase injection speed to avoid front cooling; ②keep the injection speed curve stable; ③appropriately raise the melt temperature to reduce viscosity; ④raise the mold temperature in the neck area.
Conclusão principal
Neck white spots reflect improper filling speed or temperature management; the neck no longer deforms in the blowing process, and defects from the injection stage are retained as-is, so they must be controlled at the source.
PET; preform; bottle neck; white spot; crystallization; injection speed