Injection Molding
7 visualizações
PP Short Shot
Fenómeno do problema
Material shortage at the end of thin-wall long-flow PP parts.
Análise das causas
Although PP has good flowability, thin-walled parts have high flow resistance; low melt temperature, insufficient injection speed, poor venting, and too thin walls still cause short shots.
Solução
①Increase injection speed and pressure; ②raise melt and mold temperature; ③enlarge the gate; ④improve venting; ⑤evaluate whether wall thickness is below the moldable limit.
Conclusão principal
PP short shots are mostly a balance problem of speed and venting.
Isto foi útil?
0 pessoas acharam isto útil