Menu
Materiais Máquinas
Perspetivas
Artigos Vídeos Problema e solução
About
Sobre a Chembull Parceiros de média
Contacte-nos
Idioma
EnglishالعربيةPortuguêsEspañolDeutschTürkçe한국어
Voltar a Problema e solução
Material Drying 7 visualizações

Silver streaks caused by moisture during EAA processing

Fenómeno do problema
White silver streaks appear on the surface of EAA injection molded products
Análise das causas
Raw material contains moisture >0.05%, which vaporizes during high-temperature processing to form bubbles that are stretched into silver streaks; insufficient drying or condensed moisture in the hopper
Solução
1) Dry the raw material at 80°C for 3-4h to moisture content <0.02%; 2) Increase the back pressure by 0.5-1MPa for venting; 3) Reduce the injection speed to avoid air entrainment; 4) Heat the hopper to prevent condensed moisture
Conclusão principal
Silver streaks are caused by moisture vaporization and stretching; drying and venting are the main countermeasures
EAA injection silver streak moisture drying venting back pressure

Isto foi útil?

0 pessoas acharam isto útil

ChemAI