Production & Quality
14 visualizações
EMA Performance Decay After Repeated Processing
Fenómeno do problema
After 3-4 times of recycling and reprocessing, EMA tensile strength decreases by 25-30%
Análise das causas
Molecular chains break and degrade under repeated high-temperature shear; antioxidants are exhausted in multiple processing; cumulative effect of thermo-mechanical degradation
Solução
1) Recycled material proportion not exceeding 20-30%; 2) Supplement 0.1-0.2wt% antioxidant at each re-extrusion; 3) Lower processing temperature by 5-10°C; 4) Reduce screw speed to reduce shear
Conclusão principal
Performance decay after multiple processing is caused by thermo-mechanical degradation; limiting regrind and supplementing antioxidants are key