EMA surface tiger stripes
Fenómeno do problema
Tiger stripe alternating light and dark bands 2-5mm wide on EMA injection molded product surface
Análise das causas
Unstable injection speed with melt front fluctuating fast and slow; mold temperature too low <30°C causing rapid front cooling
Solução
1) Multi-stage injection slow-fast-slow to stabilize the front; 2) Increase mold temperature to 40-50°C; 3) Increase injection pressure for stable advancement
Conclusão principal
Tiger stripes are caused by unstable injection front; multi-stage injection and high mold temperature are key