Burnt Marks from Insufficient Mold Venting in PU '2079851475616104452

Fenómeno do problema
PU injection mold venting insufficient, air in the cavity compressed and heated causing local burning
Análise das causas
Mold vent groove area insufficient or position improper; injection speed too fast, air has no time to escape; air compressed to high temperature >200°C causing oxidative burning
Solução
1) Increase vent groove area, depth 0.02-0.03mm, width 5-10mm; 2) Set vent grooves at the last-fill areas of the melt; 3) Reduce injection speed to decrease air compression; 4) Multi-stage injection with slow advancement for venting
Conclusão principal
Burning is caused by insufficient venting and high-speed injection compressing air; increasing venting and reducing speed are key