Extrusion & Post 12 visualizações

Delamination in PU Blending with Incompatible Resins

Fenómeno do problema
PU blended with polar resins such as PA/ABS, extrudate completely delaminated, mechanical properties extremely poor
Análise das causas
PU and polar resins have large polarity difference, compatibility zero, interfacial adhesion extremely low, no compatibilizer used
Solução
1) Use PU graft compatibilizer PU-g-MAH 2-5wt%; 2) Add epoxy-type compatibilizer 1-2wt%; 3) PU addition <10wt% to keep the other resin as the continuous phase; 4) Twin-screw high-shear blending to disperse PU <0.3μm
Conclusão principal
Blends with large polarity difference require reactive compatibilizer to form chemical bonding at the interface to solve it
PU blend delaminationpolarity differencePU-g-MAHreactive compatibilizationinterfacial bonding

Isto foi útil?

0 pessoas acharam isto útil