PU Extruded Film Thick Edges and Thin Middle
Fenómeno do problema
PU extruded film edges 20-30% thicker than the middle, thickness in U-shaped distribution
Análise das causas
Die flow channel design improper, edge resistance low and flow large; PU melt elasticity, swell larger at edges; air ring cooling edge effect different
Solução
1) Die with coat-hanger design to balance middle and edge resistance; 2) Fine-tune die gap slightly larger in the middle and slightly smaller at the edges for compensation; 3) Slightly reduce air volume at the air ring edges; 4) Add restrictor bar to adjust edge flow
Conclusão principal
U-shaped thickness is caused by die flow channel and swell differences; coat-hanger die and gap fine-tuning are key
Isto foi útil?
0 pessoas acharam isto útil
Obrigado pelo seu comentário!