Injection Molding 6 visualizações

Glass Fibre '2079851475616104452 flow marks

Fenómeno do problema
Glass Fibre injection molded product surface shows radial flow marks centered on gate
Análise das causas
Injection speed too fast causes melt front instability; mold temperature too low <30°C, front rapidly cools forming marks
Solução
1) Adopt multi-stage injection speed slow-fast-slow to control front stability; 2) raise mold temperature to 40-50°C to delay front cooling; 3) stabilize injection pressure to avoid fluctuation; 4) enlarge gate area to reduce pressure sudden change at gate
Conclusão principal
Flow marks are caused by injection front instability and rapid cooling; multi-stage injection and high mold temperature are key
Glass Fibre injectionflow marksinjection speedmold temperaturegate area