Extrusion & Post 17 visualizações

POE blended with incompatible resins, delamination

Fenómeno do problema
POE blended with polar resins such as PA/ABS, the extrudate completely delaminates, mechanics extremely poor
Análise das causas
POE and polar resins have large polarity differences, compatibility is zero, interfacial adhesion is extremely low, no compatibilizer used
Solução
1) Use POE grafted compatibilizer POE-g-MAH 2-5wt%; 2) Add epoxy-type compatibilizer 1-2wt%; 3) POE addition <10wt% to keep the other resin as the continuous phase; 4) Twin-screw high-shear blending to disperse POE <0.3μm
Conclusão principal
Blends with large polarity differences require reactive compatibilizers to form chemical bonding at the interface to solve it