Extrusion & Post 18 visualizaciones

POE blended with incompatible resins, delamination

Fenómeno del problema
POE blended with polar resins such as PA/ABS, the extrudate completely delaminates, mechanics extremely poor
Análisis de la causa
POE and polar resins have large polarity differences, compatibility is zero, interfacial adhesion is extremely low, no compatibilizer used
Solución
1) Use POE grafted compatibilizer POE-g-MAH 2-5wt%; 2) Add epoxy-type compatibilizer 1-2wt%; 3) POE addition <10wt% to keep the other resin as the continuous phase; 4) Twin-screw high-shear blending to disperse POE <0.3μm
Conclusión clave
Blends with large polarity differences require reactive compatibilizers to form chemical bonding at the interface to solve it
POE blend delaminationpolarity differencePOE-g-MAHreactive compatibilizationinterfacial bonding