Production & Quality
6 visualizações
POE repeated processing performance decay
Fenómeno do problema
POE after 3-4 times of recycling and reprocessing, tensile strength drops 25-30%
Análise das causas
Molecular chains break and degrade under repeated high-temperature shear; antioxidant exhausted in multiple processing; thermo-mechanical degradation cumulative effect
Solução
1) Recycled material ratio no more than 20-30%; 2) Supplement 0.1-0.2wt% antioxidant at each re-extrusion; 3) Lower processing temperature 5-10°C; 4) Lower screw speed to reduce shear
Conclusão principal
Performance decay from multiple processing is caused by thermo-mechanical degradation; limiting regrind and supplementing antioxidant are key