Injection Molding 14 visualizações

Insufficient filling/short shot in PET preform injection

Fenómeno do problema
The cavity is not completely filled during PET preform injection; the preform top is missing or the length is insufficient.
Análise das causas
Injection pressure or speed is insufficient; melt temperature is on the low side and fluidity is poor; gate size is on the small side with large resistance; venting is poor.
Solução
Increase injection pressure to 80-120MPa and increase injection speed; increase barrel temperature; enlarge gate size; improve venting.
Conclusão principal
PET preform short shot is usually related to excessive flow resistance.
PETshort shotinsufficient fillinginjection pressuregate