Molding Process
8 visualizações
Yellowing of PMMA products
Fenómeno do problema
PMMA transparent products yellow and transparency decreases.
Análise das causas
Processing temperature too high >260°C or residence time too long causes thermal degradation; PMMA depolymerizes to produce monomer MMA which is colored.
Solução
Strictly control processing temperature at 200-240°C not exceeding 260°C; shorten residence time; use stabilized PMMA grades.
Conclusão principal
PMMA thermal stability is limited; strict temperature control is the key.