Extrusion & Post
12 görüntüleme
PC extrusion sheet temperature
Sorun Belirtisi
【Problem Phenomenon】PC extruded sheet has bubbles or poor surface, improper temperature
Neden Analizi
PC extrusion melt temperature 250-290℃, slightly lower than '2079851475616104452; raw material must be fully dried; die temperature affects the surface;During on-site troubleshooting, verify item by item according to this mechanism, and avoid blindly adjusting the machine based solely on experience
Çözüm
Dry at 120℃×3-4h before extrusion; melt temperature 250-290℃; die temperature matched;After adjustment, take continuous samples to verify the effect, and resume mass production only after confirming stability
Temel Çıkarım
PC extrusion dries first, melt temperature 250-290℃;After confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence;Include this case in the defect archive as a reference for troubleshooting similar problems in the future
Bu faydalı oldu mu?
0 kişi bunu faydalı buldu
Geri bildiriminiz için teşekkürler!