Poor printing adhesion of PVA film
Sorun Belirtisi
After printing on PVA film, ink adhesion
Neden Analizi
PVA surface polarity has poor affinity with ink; corona treatment effect decays quickly; ink system does not match PVA
Çözüm
1) Print immediately after corona treatment within 24h; 2) Use PVA-specific ink; 3) Increase corona power to 15-20kW/m² to ensure surface tension >42mN/m; 4) Flame treatment to assist surface polarization
Temel Çıkarım
Poor printing adhesion is caused by insufficient surface polarity; corona treatment and dedicated ink are the key