Extrusion & Post 5 görüntüleme

POE extrusion film longitudinal streaks

Sorun Belirtisi
POE extruded film surface shows continuous streaks along the extrusion direction, width 1-3mm
Neden Analizi
Local damage to die lip or uneven gap; melt residence zone inside the die produces unstable flow; pressure fluctuation at the screw front end
Çözüm
1) Check die lip flatness and gap uniformity ±0.01mm; 2) Clean the die interior to remove carbonized material in the residence zone; 3) Install a gear pump on the extruder to stabilize melt pressure; 4) Polish die lip to Ra<0.1μm
Temel Çıkarım
Longitudinal streaks are caused by die defects and pressure fluctuation; die maintenance and pressure stabilization are key