Extrusion & Post 10 görüntüleme

POE extruder screw severe wear

Sorun Belirtisi
After 200h of POE extrusion, screw and barrel wear reaches 0.5mm
Neden Analizi
Filler causes large wear to the screw; screw material hardness insufficient, not nitrided; processing temperature too high causes POE to adhere to the screw, aggravating wear
Çözüm
1) Use nitrided screw or bimetallic screw SK-2 alloy; 2) Lower processing temperature to reduce adhesive wear; 3) Treat filler with coupling agent to reduce friction; 4) Regularly check wear, replace promptly when >0.3mm
Temel Çıkarım
Screw wear is caused by filler friction and adhesion; wear-resistant screw and temperature control are key