Molds & Tooling
5 görüntüleme
High fiber content product filling difficulty
Sorun Belirtisi
LGFPP with fiber content >40% has extremely poor flowability, and thin-wall products cannot be filled completely
Neden Analizi
Fibers form a physical network structure restricting PP molecular chain movement; friction resistance between fibers greatly increases the apparent viscosity of the system; fibers hinder melt flow in the cavity
Çözüm
Appropriately increase the processing temperature to improve flowability (not exceeding the degradation temperature of 240°C); add processing aids to reduce inter-fiber friction; reduce fiber content to 30-35% or shorten fiber length
Temel Çıkarım
Fiber content and processing flowability conflict with each other within a certain range and need to be balanced