Injection Molding 5 مشاهدة

EEA injection warpage deformation

ظاهرة المشكلة
EEA injection molded products warped 2-3mm/100mm after demolding, flatness not up to standard
تحليل الأسباب
EEA shrinkage rate large and mold temperature uneven causing shrinkage difference in all directions; improper gate position, flow orientation stress unevenly released; insufficient cooling time
الحل
1) Increase mold temperature to 40-60°C to reduce temperature difference; 2) Increase holding pressure to 50-70MPa; 3) Optimize gate position for uniform flow; 4) Extend cooling time; 5) Anneal to release residual stress
الخلاصة الأساسية
Warpage is caused by shrinkage difference and orientation stress; uniform mold temperature and holding are the key
EEA injectionwarpageshrinkage rateholding pressureannealing treatment

هل كان هذا مفيدًا؟

0 شخص وجدوا هذا مفيدًا